Hot Washing Machine: Caustic Dosing and Temperature

Temperature, caustic concentration and dwell time act as one control window on a hot wash. Where each edge sits, and how drift shows up in the pellet.

Temperature, caustic concentration and dwell time are one control window, not three settings: 85-95 degrees C, 1-2% caustic soda of the water volume, and 30-45 minutes per batch. Move one and the tolerance on the other two moves with it.

Each edge has a defined failure. Below the band the adhesive survives; above it the alkali starts working on the PET. Downstream the window is readable in the pellet: yellow foam means the caustic drifted, brittle low-IV pellets mean the moisture did.

Three dials, one window

  • 85-95 degrees C, 1-2% caustic of the water volume, 30-45 minutes per batch.
  • Below the band the glue survives; above it the alkali attacks the PET.
  • Caustic is used up and carried away, so the tank drifts through a batch.
  • Yellow foam and brittle pellets are the two downstream readings of the window.
3D product render of a TENGLONG plastic pelletizing machine on a white background, shown here as a visual reference for caustic dosing and temperature control.
3D product render of a TENGLONG plastic pelletizing machine on a white background, shown here as a visual reference for caustic dosing and temperature control.. Used here as a visual reference for the caustic dosing and temperature control of a hot wash tank. Rendering, not a photograph of a customer plant.

Three Variables That Cannot Be Set Alone

A hot caustic wash is one of the few stages on a plastic recycling equipment line where the operating window is a chemistry problem rather than a mechanical one. Three variables control it: temperature, caustic concentration and dwell time. The published window is 85–95 °C, 1–2% caustic soda of the water volume with a surfactant, and 30–45 minutes per batch.

Those three numbers only work together. Move one of them and the tolerance on the other two moves with it, which is why this is a window and not three independent settings on a panel. A buyer who reads 85 °C, 1.5% and 30 minutes as three numbers to confirm on delivery has misunderstood the whole stage: the same concentration behaves differently at the bottom of the temperature band than at the top.

The useful way to write the spec is as a band with a defined failure at each edge. Below the bottom edge the adhesive stays on the flake. Above the top edge the alkali starts working on the PET instead of only on the glue. The window is the space between those two failures, and the dose, the heat and the clock are the three things that hold it open.

Temperature: Where the Energy Goes and Where the Risk Sits

Rendered factory scene with TENGLONG plastic pelletizing machine and operators on the plant floor, shown here as context for a machine installation in a plant hall at a hot washing machine.
Rendered factory scene with TENGLONG plastic pelletizing machine and operators on the plant floor, shown here as context for a machine installation in a plant hall at a hot washing machine.. Shown here as production context. Rendering, not a photograph of a customer plant.

Heating the bath is the reason a hot wash costs more to run than a cold one. Published energy use for a washing line is 18–30 kWh per ton of flake, and most of that goes into keeping water at temperature rather than into the pumps and the agitation. Water is the heat store, and the heater has to replace what the tank loses into the shell and into the wet flake.

85 °C is a working floor, not a nominal. At the low edge of the band the adhesive releases slowly, the batch still finishes, still looks clean, and still leaves a residue that shows up downstream. 95 °C is the working ceiling for the mirror-image reason: above it the alkali works on the PET, and PET that has been attacked carries the damage into the pellet where nobody can see it.

Temperature also has to hold across the batch rather than merely be reached. A tank that is at setpoint when the flake goes in and a few degrees below when the flake comes out has been running a different process for most of the cycle. The setpoint is not a target to hit once at the start of a batch. It is a condition to keep from the first charge to the last.

Caustic: A Percentage of Water, Dosed Into the Loop

Caustic is dosed at 1–2% of the water volume and dosed from a concentrated tank into the heated water loop. Two parts of that sentence matter more than they look. The percentage is of water, so it moves whenever the tank is filled to a different level, and the dose point sits in the heated loop so that the detergent enters where it actually mixes with the bath.

Caustic is also a consumable, and this is the part that catches people out. It is used up by the contamination it is dissolving and carried out with the wash water, so the concentration inside the tank falls through a batch even when the opening dose was correct. A tank dosed once at the start and recirculated for the rest of the cycle will drift, and the drift is invisible until the flake is in the dryer.

Where the tank sits inside the window matters as much as the number. Below the band the glue survives the tank and reaches the dryer as a residue that is much harder to remove afterwards than it would have been in the tank. Above the band, the same heat and the same PET produce a different flake surface, and every downstream stage inherits that difference all the way to the pellet.

Dwell Time: The Variable Throughput Steals

Dwell time is published at 30–45 minutes per batch, and it is the one of the three that the plant steals rather than the plant sets. Once a tank is built, the time a batch spends in it is fixed by how much material you push through it per hour. Run the line faster and the dwell shortens, and no amount of adjusting the temperature or the dose will put it back.

This is why the dwell time belongs in the sizing decision rather than in the operating instructions. A tank specified for the fast case will under-wash the difficult one, and the difficult material is exactly the material that got a buyer interested in a hot wash in the first place. The published performance figure for real washing-line throughput is 60–80% of nameplate, which is the range most plants actually live in.

If a plant needs more dwell than its tank gives, there are only two honest answers: slow the line down, which costs output, or buy a bigger tank, which costs capital and space. There is no third answer, and any supplier who offers one is describing a controller setting rather than a process.

Reading the Window From the Finished Pellet

The window is not visible inside the tank. It is visible in the pellet, which is why the link between the wash stage and the extrusion stage has to be written into the quality control routine rather than left to whoever is on shift. A flake pH below 8.0 keeps residual caustic from foaming the melt and yellowing the pellet, and flake moisture below 0.5% is the condition for stable extrusion.

White specks in a customer’s pellet usually come back to this stage, and the first question a PET pelletizing line owner asks is usually about the screw. It is not the screw and it is not the screen change interval. It is alkaline flake that never got rinsed back, and it arrives at the extruder as foam in the melt and as poor colour in the pellet. A complaint about specks gets answered by sampling the flake, not by changing the screw.

So the downstream readings separate the failure modes. A yellow, foamy pellet means the caustic side of the window drifted. A brittle pellet with low intrinsic viscosity means the moisture side drifted, because water in wet flake triggers hydrolysis in the melt and permanently breaks the polymer chain. Both are cheap to catch at the rinse and expensive to catch at the extruder. The terminology matters, so the plastic pellets glossary is worth a read before a specification sheet is written.

The control window, its setpoints and what each edge costs

Temperature, concentration and dwell time are one control loop, not three settings. The table shows the window and what happens outside it.

Parameter Published target What the low edge costs What the high edge costs
Wash temperature 85–95 °C Adhesive does not release Caustic starts working on the PET
Caustic concentration 1–2% of water volume Glue survives into the dryer Flake surface is attacked at heat
Dwell time 30–45 minutes per batch Batch leaves with residue Heat load and energy per ton rise
Flake pH after the rinse Below 8.0 Low pH is safe: 8.0 is a ceiling Foaming and yellowing in the melt
Flake moisture after drying Below 1–2% Drier flake, still acceptable Hydrolysis in the melt, brittle pellets

Frequently asked questions

Q1: Why can temperature, caustic and dwell time not be set independently?

Because they are coupled. The published band is 85–95 °C with 1–2% caustic soda and a surfactant for 30–45 minutes per batch. The same concentration behaves differently at the bottom of the temperature band than at the top, and the same temperature does less work at 30 minutes than it does at 45.

Q2: Is caustic dosed as a percentage of the flake or of the water?

Of the water volume: 1–2% caustic soda, drawn from a concentrated tank and dosed into the heated water loop. Caustic is also used up as it dissolves contamination and carried out with the wash water, so the concentration inside the tank falls through a batch and has to be measured rather than assumed.

Q3: What happens if the wash runs above 95 °C?

Above the published band the alkali starts working on the PET rather than only on the adhesive. That damage happens inside the tank and travels into the pellet, where it cannot be seen, measured or undone after the fact.

Q4: How does a bad wash show up in the finished pellet?

As foam and yellowing if the caustic side drifted, because a flake pH below 8.0 is what keeps residual caustic out of the melt. If the pellet is brittle with low intrinsic viscosity instead, the moisture side drifted and hydrolysis has been breaking the polymer chain.

The rest of this series covers the same equipment from different angles: Hot Washing Machine for PET: What It Actually Removes, Sizing a Hot Washing Machine: Tank Volume and Turnover, Hot Washing Machine vs Cold Wash: Cost per Tonne and Hot Washing Machine Acceptance and First-Week Faults.

About the author

Zhou Gong (周工) is a recycling machinery engineer at TENGLONG Plastic Machinery in Linyi, Shandong, where 30-plus staff work across 18,000 m² and 12 machine platforms covering 100 to 3,000 kg/h. I do not judge a hot wash by the tank temperature alone; I judge it by what the pellet looks like a week after the rinse. Every figure used here has been measured on a machine or taken from a dated published source, not from a brochure.

Send the material form, the contamination level and your target output to our engineering team and you get a model and a price range within one working day. A test run on 10-20 kg of your own material is free, and if the measured output misses the agreed figure by more than 5%, the deposit is refundable.

Related reading

العربيةAR