Technical notes · · 6 min read
Strand, water ring or underwater: which cutting method
Pellet shape, floor space, dust level, polymer suitability and price — the same comparison we run with every buyer.
Strand cutting gives cubic pellets and a visible melt, and needs 8–12 m of length. Water ring cuts at the die face inside a ring of water and needs 5–7 m. Underwater cuts in a pressurised chamber and needs 6–8 m but produces the roundest, cleanest pellet. The right choice is decided by the pellet your customer buys.
| Criterion | Strand | Water ring | Underwater |
|---|---|---|---|
| Pellet shape | Cubic, sharp edges | Rounded | Spherical |
| Floor length | 8–12 m | 5–7 m | 6–8 m |
| Fines level | 0.5–1.5% | 0.3–0.8% | below 0.2% |
| Best polymers | PP, PE, ABS, PVC | PP, PE, filled PP | PET, PA, masterbatch |
| Operator attention | High (strand breaks) | Medium | Low |
| Relative price | 1.0 | 1.3 | 1.8 |
Why PET cannot run on a strand line
Amorphous PET crystallises on the surface as it cools in air, so a strand becomes brittle and snaps at the first guide roll. Underwater cutting quenches the pellet in milliseconds, keeping the surface amorphous and the pellet ductile. The same logic applies to PA, which absorbs moisture from the air bath within seconds.
A note on pellet shape and feeding
Cubic pellets from strand cutting feed more predictably in injection machines because they interlock less; round pellets flow better in pneumatic conveying and cause fewer bridging problems in silos. If your customer complains about hopper bridging, round is better; if they complain about feed-zone surging, cubic is better.
Questions buyers ask
Can I change cutting method later?
On the same extruder frame, yes — water ring and strand share the die flange, so a swap is a mechanical change plus a control parameter. Underwater needs a different chamber and dryer, so it is better decided at order stage.
Which is best for filled PP with 40% CaCO3?
Water ring. The filled melt is abrasive and sets fast; die-face cutting in a ring avoids the strand breakage you would get in a bath, and the round pellet conveys well in a dosing system.