Keeping IV loss under 0.03 dl/g on an rPET line

Moisture, temperature and residence time: the three variables that decide whether recycled PET can go back into a bottle.

PET pelletizing line with crystallizer and underwater pelletizer

Intrinsic viscosity falls by about 0.006 dl/g for every 100 ppm of moisture in the melt. Keep feed below 50 ppm, melt at 275–285 °C and residence under 90 seconds, and a single pass loses 0.02–0.03 dl/g — which is what a bottle-to-bottle line can afford.

1. Moisture: crystallize before you dry

Amorphous PET softens at 75 °C, so flake put straight into a 160 °C dryer fuses into a block. Crystallisation at 140–160 °C for 20–30 minutes raises the softening point above 200 °C, after which a −40 °C dew-point hopper can dry to 50 ppm in four to six hours. Skipping crystallization is the most common cause of a blocked dryer and a burnt batch.

2. Temperature: melt gently, do not over-mix

Above 290 °C, thermal degradation accelerates sharply; below 270 °C, unmelted flake raises torque and forces the operator to overheat the last zones. The stable window is 275–285 °C with a 32:1 deep-flighted screw and low-shear mixing elements. A high-shear screw designed for compounding will destroy IV even at correct temperature.

3. Residence time: keep the flow path short

Every extra 30 seconds above 280 °C costs roughly 0.005 dl/g. That means no oversized melt pump, no unnecessary static mixer, and a die with the minimum practical land length. On a 1,000 kg/h line the difference between a 70-second and a 120-second path is about 0.008 dl/g per pass — visible in the final bottle test.

What to measure, and how often

  • Feed moisture: every batch, halogen meter, target below 50 ppm.
  • Melt temperature at the die: continuous, alarm at 290 °C.
  • IV: every 4 hours by solution viscometry, trend charted.
  • Acetaldehyde for bottle grades: daily, target below 3 ppm.

Questions buyers ask

Can I raise IV back up after pelletizing?

Yes, with solid-state polycondensation (SSP) at 200–220 °C under vacuum or nitrogen, which typically adds 0.05–0.15 dl/g. But SSP is a separate plant and cost; it is cheaper to lose less IV in the first place.

Does pellet colour predict IV loss?

Partly. Yellowing (higher b*) usually accompanies thermal degradation, but moisture-driven hydrolysis can occur with little colour change. Colour is a warning, not a measurement — measure IV.